Table of Contents
- ASTM D638: Scope of Evaluation and Limits of Application
- ASTM D638 test specimens: Errors can begin during fabrication
- Measuring the specimen cross-section
- ASTM D618: Conditioning practices
- Testing speed and the mechanical response of polymers
- Alignment, grips, and extensometers: Sources of misleading data
- From the Stress-Strain Curve to defensible test results
- How to reduce differences between testing laboratories
- Conclusions
- References
- Frequently Asked Questions (FAQs)
Two test specimens made from the same polymer can produce different stress-strain curves, even when both are tested in accordance with ASTM D638. The source of these differences is not always the material itself. Specimen geometry, conditioning, alignment, gripping, strain measurement, and testing speed can introduce variations that affect the measured tensile strength, modulus, or elongation.
Therefore, reliable tensile testing of plastics requires control over the entire process. The testing machine applies the load, but the validity of the results begins before testing, with proper specimen selection and preparation, and ends with a consistent interpretation of the resulting stress-strain curve.
ASTM D638: Scope of Evaluation and Limits of Application
ASTM D638-22 establishes the test method for determining the tensile properties of reinforced and unreinforced plastics using standardized specimens tested under defined conditions of pretreatment, temperature, humidity, and testing machine speed.
The properties that can be determined include:
- Tensile strength: The maximum tensile stress reached during the test.
- Yield stress: The point at which significant deformation begins without a proportional increase in load.
- Elongation: The extent to which the specimen can deform during testing.
- Modulus of elasticity: The initial relationship between stress and strain.
- Poisson’s ratio: When the measurement configuration allows its determination.
ASTM D638 covers materials up to 14 mm thick. For thin plastic sheeting and films less than 1.0 mm thick, ASTM D882 is the preferred test method. Elastomers are covered by ASTM D412, while high-modulus fiber-reinforced composites are addressed by ASTM D3039/D3039M.
Selecting the appropriate test method helps prevent comparisons between results obtained using different specimen geometries, testing speeds, and deformation mechanisms. ASTM D638 and ISO 527-1 have a similar scope of application but differ in their technical requirements.
ASTM D638 test specimens: Errors can begin during fabrication
The dog-bone geometry concentrates deformation within a reduced cross-section and keeps fracture away from the grips. ASTM D638 specifies five specimen types, with selection depending on material thickness, material behavior, sample availability, and the purpose of the test.
The following video demonstrates the injection molding process used to manufacture an ASTM D638 Type IV plastic test specimen. This manufacturing step illustrates how specimen geometry and preparation form part of the quality controls performed before tensile testing.
ASTM D638 test specimens can be produced by molding, die cutting, or machining. Each manufacturing process may introduce conditions that affect the test results:
- Burrs or notches: Act as localized stress concentrators.
- Machining damage: May initiate fracture before the material exhibits its characteristic mechanical response.
- Thickness variations: Change the cross-sectional area used to calculate stress.
- Molecular orientation: An injection-molded specimen may retain flow-induced orientation effects.
- Residual stresses: Manufacturing processes may influence the material’s response under loading.
Comparing results without documenting specimen preparation can make it difficult to distinguish the inherent mechanical behavior of the polymer from effects introduced during manufacturing.
Measuring the specimen cross-section
Engineering stress depends on the measured force and the original cross-sectional area:
σ = F / A₀
Therefore, an error in width or thickness measurement directly affects the calculated stress. A specimen that is thinner than its recorded dimensions will appear to have a different tensile strength, even if the maximum force recorded by the testing machine is correct.
ASTM D5947-24 establishes methods for determining the physical dimensions of plastic specimens when those dimensions are used to calculate material properties. For die-cut or machined specimens, local dimensional variations justify measuring each ASTM D638 specimen individually. For molded batches, sufficient dimensional repeatability must be demonstrated before assuming that a single measurement represents the entire batch.
It is important to verify that the measuring instrument and its contact pressure do not deform soft materials during measurement. Specimen width and thickness directly determine the area used in stress calculations, making dimensional traceability an integral part of the test results.
ASTM D618: Conditioning practices
Temperature and humidity can affect the mechanical response of many polymers. Moisture absorption, for example, can influence stiffness, yield behavior, and elongation. Two specimens made from the same material but stored under different conditions may not be in the same condition when testing begins.
ASTM D618-21 establishes practices for conditioning plastics before testing and controlling the conditions under which testing is performed, with the objective of improving reproducibility and comparability. A material-specific specification may establish different conditions that take precedence over the general practice.
Conditioning should not automatically be interpreted as achieving complete equilibrium with the surrounding environment. Depending on the material, thickness, and previous exposure history, reaching equilibrium may require extended periods. Consistently applying ASTM D618 and documenting conditioning conditions helps distinguish material-related variations from those introduced by storage or preparation.
Testing speed and the mechanical response of polymers
Plastics exhibit viscoelastic behavior, meaning that their mechanical response depends on both the magnitude of deformation and the rate at which that deformation occurs. Changing the testing speed can affect the modulus, yield stress, maximum stress, and elongation.
ASTM D638 specifies different testing speeds depending on the material and its expected behavior. The speeds used under the standardized procedure cover a broad range, approximately 1 to 500 mm/min, depending on the applicable conditions. Using a single testing speed for all polymers eliminates one setup variable but does not ensure technically comparable results.
Increasing the testing speed may cause certain plastics to exhibit higher apparent stiffness or strength and reduced deformability. The magnitude of this effect depends on the polymer. Consequently, tensile strength measured at a given testing speed should not be directly compared with data obtained at a different speed without verifying the test conditions.
To obtain reproducible results, the testing speed must be selected according to ASTM D638 requirements and the applicable material specifications. This parameter must be correctly configured on the testing machine and recorded with the results. When the procedure requires changes in testing speed during specific stages, those changes must also be applied and documented consistently.
Alignment, grips, and extensometers: Sources of misleading data
A calibrated testing machine cannot compensate for an improperly mounted specimen. If the specimen’s longitudinal axis is offset from the line of loading, additional bending stresses develop, and the stress distribution no longer corresponds to the expected uniaxial tensile loading conditions.
Specimen gripping presents another balance. Insufficient gripping pressure allows slippage, while excessive pressure may leave marks, crush the material, or cause damage near the grips. Repeated fractures near the gripping region should prompt a review of alignment, gripping pressure, grip faces, and specimen preparation before the results are accepted as representative.
Strain measurement also requires careful attention. Crosshead displacement includes deformation and movement within the testing system that do not necessarily correspond to the actual strain within the specimen’s gage length. For sensitive properties such as modulus, using an appropriate extensometer reduces this uncertainty.
For modulus measurements and low-strain measurements, the technical requirements of ASTM D638 call for extensometer accuracy consistent with ASTM E83 Class B-2. For soft materials or those exhibiting high elongation, it is also necessary to assess whether a contact extensometer may influence specimen behavior and whether an optical measurement system would be more appropriate.
Fracture outside the expected region also provides useful information
The fracture location can reveal problems with the test setup. If several specimens fail near the grips, exhibit similar damage at their ends, or show abnormal behavior at the beginning of their stress-strain curves, simply recording the maximum value and continuing is insufficient.
Before accepting these results, the following aspects should be verified:
- Alignment: Confirm that the specimen axis coincides with the line of loading.
- Gripping: Verify that no slippage or grip-induced damage occurs.
- Geometry: Confirm specimen dimensions and the transition into the reduced section.
- Preparation: Check for burrs, notches, or machining damage.
- Strain measurement: Verify the extensometer signal and its measurement gage length.
These checks allow abnormal fracture behavior to serve as an indication of process-related issues rather than automatically including the corresponding results in an average.
From the Stress-Strain Curve to defensible test results
Data acquisition ends when the specimen fractures, but the tensile testing process is not yet complete. The stress-strain curve must be reviewed to identify yielding, maximum stress, strain, fracture, and the region used to calculate the modulus.
A common problem occurs in the initial portion of the curve. Mechanical clearances, grip seating, or settling of the testing system can produce an initial region that does not represent the material’s elastic response. ASTM D638 provides for toe compensation when this effect occurs, because including the initial displacement in the calculations can alter the modulus, strain, and certain yield-related values.
Another error can occur when reporting strain after yielding. When the material exhibits necking, deformation is no longer uniformly distributed along the specimen. Under these conditions, strain measured by the extensometer must be distinguished from the nominal strain defined by ASTM D638 for the applicable calculation, because using an incorrect measurement source can affect the reported elongation.
Consistent calculation criteria must also be maintained. Tensile strength represents the maximum stress reached, while yielding, strain at break, and modulus describe different aspects of the material’s response. Selecting an isolated value without examining the shape of the curve may conceal significant differences between formulations or production batches.
Comparisons become more meaningful when test reports retain sufficient information to reconstruct the test: material identification, batch identification, specimen geometry, dimensions, conditioning, temperature, humidity, testing speed, testing equipment, strain measurement system, and failure mode.
How to reduce differences between testing laboratories
Reproducibility requires control over the entire process that transforms a specimen into a test result. The first step is to confirm that ASTM D638 is appropriate for the material, select the proper specimen geometry, prepare and measure the specimens, and apply ASTM D618 or the relevant conditioning specification.
The test setup must maintain equivalent criteria for testing speed, grips, alignment, and extensometry. During testing, slippage, asymmetric deformation, damage near the grips, or repeated fractures outside the expected region should be investigated before expanding the testing program.
Comparing laboratories also requires comparing test conditions. Two sets of results may both be reported as obtained “in accordance with ASTM D638” while originating from different specimen geometries, testing speeds, environmental conditions, or measurement systems. Documenting these variables provides a more reliable basis for determining whether observed differences result from the material or the testing procedure.
Conclusions
Reliable tensile test results depend on more than the testing machine’s ability to apply force. Specimen geometry and dimensions, conditioning, alignment, the gripping system, strain measurement, and testing speed influence the measured values, even when the same material is tested.
ASTM D638 establishes procedures for evaluating the tensile properties of plastics. Complementary standards, such as ASTM D618, which addresses specimen conditioning, and ASTM D5947, which covers the measurement of physical specimen dimensions, help control testing conditions and obtain comparable results.
Traceability of each result to the tested specimen and the specific test conditions allows proper interpretation of the stress-strain curve. This information supports quality assessment, material selection, and engineering decision-making.
References
- ASTM International. ASTM D638-22, Standard Test Method for Tensile Properties of Plastics.
- ASTM International. ASTM D618-21, Standard Practice for Conditioning Plastics for Testing.
- ASTM International. ASTM D5947-24, Standard Test Methods for Physical Dimensions of Solid Plastics Specimens.
- ASTM International. ASTM D882-26, Standard Test Method for Tensile Properties of Thin Plastic Sheeting.
- ASTM International. ASTM D3039/D3039M-17(2025), Standard Test Method for Tensile Properties of Polymer Matrix Composite Materials.
Frequently Asked Questions (FAQs)
What properties can be determined using ASTM D638?
ASTM D638 can be used to determine properties such as tensile strength, yield stress, elongation, and modulus of elasticity under the conditions specified by the test method.
Why does ASTM D638 specify different specimen types?
Because specimen geometry, thickness, material availability, and behavior during testing may require different configurations to obtain representative failure behavior.
Can testing speed affect tensile test results?
Yes. Plastics are sensitive to strain rate, so changing the testing speed can affect stiffness, strength, yield behavior, and elongation.
How are ASTM D618 and ASTM D638 related?
ASTM D618 establishes conditioning practices for plastics that help control the effects of temperature and humidity before testing and when comparing test results.